can't find my glasses right now, but is that mig or tig?? if tig, you're going too hot and WAY too much filler. start low on your amps and increase as necessary to maintain a decent weld puddle. if fitment is perfect, no filler is required and you can just fuse them. try to only have 90% penetration to keep contamination from the back of the weld down. i would try starting at 40 amps, smallest tungsten you have ground down to a SHARP point, and use .030 or .035 filler (unless you have access to smaller).
|